Machining notes

Spheroidize annealed260 HB

Turning

CutSFMFeed, IPRDepth, in
Finishing661450–931201 m/min0.0070.004–0.0100.18 mm/rev0.0220.004–0.0400.6 mm
Medium555379–782169 m/min0.0140.007–0.0200.34 mm/rev0.0850.012–0.1582.2 mm
Roughing522356–735159 m/min0.0170.010–0.0240.43 mm/rev0.1490.060–0.2373.8 mm

For a CVD carbide insert, general stability, 15 min tool life.

Milling, solid carbide end mill

Speed 231 (138–323) SFM · 70 m/min

Chip load per tooth, before chip thinning
Cutter ØIPTmm/tooth
1/8"0.00060.0005–0.00060.014
1/4"0.00160.0015–0.00170.041
1/2"0.00290.0028–0.00300.074
3/4"0.00420.0033–0.00500.105
1"0.00510.0041–0.00600.128

Drilling, Ø1/2" at 3×D

DrillSFMFeed, IPR
HSS7445–1150.01130.0070–0.0150
Cobalt9355–1150.01130.0070–0.0150
Solid carbide, through-coolant362265–6200.00970.0040–0.0153

Feeds scale with drill Ø (0.5" here): the drilling calculator sets them for yours.

Tapping

Cut tap
58 (40–80) SFM
Form tap
20 (10–35) SFM

Hardened 60 HRC60 HRC

Cuts as ISO H (Hardened)

Turning

Hard turning (ISO H, hardened steel) data isn’t sourced yet.

Milling, solid carbide end mill

Hardened steel (ISO H) milling data isn’t sourced yet.

Drilling, Ø1/2" at 3×D

DrillSFMFeed, IPR
HSSHardened steel needs a carbide drill
CobaltHardened steel needs a carbide drill
Solid carbide, through-coolant10870–1710.0020

Feeds scale with drill Ø (0.5" here): the drilling calculator sets them for yours.

Tapping

No sourced tapping speed for hardened steel yet.